Oil return and bubbling2

Aug 16, 2025

Leave a message

Phenomenon:
After the hot transfer film is printed, small bubbles of different sizes appear on the adhesive back surface, and there are cracking marks.


Possible causes in order:
① Insufficient pre-baking time or insufficient temperature;
② After shaking the powder, the oven temperature is too high, the surface layer of the hot melt adhesive powder dries too quickly, and the solvent in the ink is sealed in the hot melt adhesive before drying, resulting in bubbling;
③ The top coating is damp, causing ink flow and bubbling at the ink flow
④ Ink and film are incompatible


Workaround:
The front, middle and back heating of the printer needs to be turned on and kept at about 45 °C
increase the baking time, increase the oven length, and set the baking temperature at 130-150 DEG C

If the heat transfer film is affected by trend ink, please pull the outer ring off 5-10m before printing

 

info-1000-635

 

Send Inquiry